Die casting A356 T6 heat treatment process, deformation control, and mechanical property control

  • мнения: ...
  • Время выпуска: 2026-11-07

Die casting A356 T6 heat treatment process, deformation control, and mechanical property control
A356 is the main alloy for wheel hubs and structural components, with T6 solid solution and aging to enhance strength, elongation, and hardness; But heat treatment is prone to deformation, foaming, and size deviation, which is the core control process for foreign trade wheel hub orders.
1、 T6 complete process
Solution treatment: insulation at 535-545 ℃, with insulation duration according to wall thickness; Rapid water quenching; Artificial aging: insulation at 150-170 ℃ for 4-6 hours. Solid solution allows Mg2Si to dissolve into the aluminum matrix; Aging precipitation strengthens the phase and achieves the target mechanical properties.
2、 Root cause of heat treatment foaming
Internal pores and subcutaneous bubbles in castings, gas expansion and bulging at high temperatures; For products with severe gas entrapment in die-casting, batch foaming and scrapping after T6, X-ray pre screening is a common method in foreign trade.
3、 Deformation control measures
Fixture shaping quenching; The quenching water temperature and water inlet speed are stable; Choose rigid positions for the support points of the casting runner and fixture; The uneven thickness of the parts reduces the heating rate and minimizes thermal stress.
4、 Mechanical performance boundary
Qualified T6 A356: Tensile strength ≥ 220MPa, yield ≥ 160MPa, elongation ≥ 6%; Insufficient insulation and strength; Excessive insulation results in coarse grains and decreased toughness.
5、 Front fitting of mold end
Reduce internal porosity in castings; Reasonably arrange the gate to compensate for shrinkage and reduce looseness; The casting is designed with uniform wall thickness to reduce heat treatment deformation caused by sudden thickness changes; Reserve allowance for heat treatment shrinkage deformation.
6、 Key points of foreign trade customer complaints
Bubbling, deformation, and failure to meet elongation standards; Many overseas customers require the attachment of heat treatment furnace temperature curves and mechanical sample reports. Google's A356 T6 heat treatment for die casting is aimed at heat treatment engineers.
FAQ
Can ADC12 do T6?
ADC12 is not suitable for T6 as it has poor reinforcement effect and is prone to foaming.
2. Water quenching causes significant deformation, can air cooling be used?
The air cooling speed is insufficient and the strength does not meet the T6 standard.
What will happen after T6 shrinkage casting?
Shrinkage will connect, and air tightness will directly leak.
4. Is the heat treatment deformation caused by the deformation of the casting itself or by the fixture?
Both are present, with uneven thickness being the internal cause and quenching impact being the external cause.
What will happen if the solid solution temperature exceeds the limit?
Overheating, coarse grains, and brittle castings.
6. Is it possible to perform advanced processing and reheating?
Generally, machining after heat treatment will consume the machining allowance due to deformation caused by heat treatment.
7. Can the bubbles generated during heat treatment be seen during the die-casting stage?
Subcutaneous stomata may not be clearly visible on X-ray, and only become apparent after T6.
8. Are the low pressure A356 wheel hub T6 and high pressure parameters the same?
Consistent alloy, close heat treatment window, less porosity in low-pressure castings, and lower risk of foaming.

сайт: https://ru.zj-xinfeng.com/news/1460.html
Не могу найти никакого контента

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Формы для литья под низким давлением (LPDC) 
Формы для гравитационного литья 
Формы для литья под противодавлением (CPC) 
Формы для литья конструкционных деталей
Форма для литья ступицы колеса мотоцикла
Форма для литья ступицы колеса под дифференциальным давлением
Форма для гравитационного литья ступицы колеса
Форма для литья ступицы колеса под низким давлением

ФОРМЫ ДЛЯ АВТОМОБИЛЬНЫХ КОЛЕС 
КОНСТРУКЦИОННЫЕ ДЕТАЛИ ДЛЯ АВТОМОБИЛЕЙ 
ДРУГИЕ АЛЮМИНИЕВЫЕ ЛИТНЫЕ ДЕТАЛИ

НОВОСТИ КОМПАНИИ
НОВОСТИ ОТРАСЛИ
ТЕХНИЧЕСКИЙ БЛОГ
ЧАСТО ЗАДАВАЕМЫЕ ВОПРОСЫ

ПРОФИЛЬ КОМПАНИИ
ОРГАНИЗАЦИОННАЯ СТРУКТУРА
ИСТОРИЯ РАЗВИТИЯ
ИНТЕЛЛЕКТУАЛЬНАЯ СОБСТВЕННОСТЬ
КОМАНДНЫЙ ДУХ И ПАРТНЕРЫ

Авторские права © Zhejiang Xinfeng Machinery Co., Ltd. Все права защищены.